Page 55 - QRedition5.0 062021
P. 55
Quality Requirements Edition 5.0 European Enamel Association
7.14.3 Quality requirements
Test method Requirement Remarks Frequency
4.3 thickness enamel coating max. 0.40 mm not applicable if covered with several S4/AQL 6.5
colour layers in order to achieve special
2
decorative effects (when coil production, 1 x per 100 m )
4.4 cold citric acid class A when taking into production a sig.diff.
enamel recipe, but at least 1 x per year
4.9 impact resistance at 20 N no damage > 2 mm diameter after 24 hours when taking into production a sig.diff.
enamel recipe, but at least 1 x a year
4.10 adherence min. 3 on test sheets may be conform in production 1 x a day
to EN ISO 28764
4.18 scratch resistance 7 N when taking into production a sig.diff.
min. 4 N for metallic finishes and silk-screened finishes enamel recipe (exclusive colour oxides),
but at least 1 x a year
4.26 abrasion resistance max. 0.1 gram conform to ASTM C 501 when taking into production a sig.diff.
sandpaper S33/1kg/1000 rotations enamel recipe (exclusive colour oxides),
ISO 6370-1 and ISO 6370-2 but at least 1 x a year
4.28 steel quality in accordance with norm EN 10209 is recommended: determination during design
DC01EK / DC04EK / DC04ED
© EEA2020 page 55